Resin sand process producing flywheel, material HT300, slight shrinkage porosity in the casting below the pressed-edge riser — cause analysis

Warm Tip: If you want to know more details about our construction services, materials, or project solutions, please contact us for a free consultation.

HT300 Flywheel, Resin Sand Process — Shrinkage Porosity Analysis Below the Riser

First, let’s look at the average spectral composition: C: 3.19%, Si: 1.90%, Mn: 0.970%, P: 0.0622%, S: 0.0535%, Cr: 0.253%, Cu: 0.0771%, Sn: 0.0052%

I. First, determine whether there is a composition-level problem

HT300 is a high-grade gray iron that relies on a pearlite matrix + a small amount of Cr to stabilize pearlite. Carbon equivalent CE = C + Si/3 ≈ 3.19 + 1.9/3 = 3.82%

  1. Carbon equivalent is on the low side: The conventional CE recommendation for HT300 is 3.85–4.0. At 3.82, it is at the lower limit. Graphitization expansion is weak, self-feeding capacity is insufficient, and shrinkage porosity is very likely to form at hot spots at the riser root.
  2. Sulfur 0.0535%: For the resin sand process, the suitable S range is 0.04–0.06, and this S value is right at the critical boundary. If S is too low, inoculation effectiveness is poor, the amount of graphite is low, and graphitization expansion is weak; if S is too high, gas porosity is likely to occur. The current value is barely acceptable.
  3. Alloying elements: Cr 0.253% is used to stabilize pearlite and improve strength, which is beneficial, but Cr slightly increases the solidification shrinkage tendency and places higher demands on feeding. Cu and Sn contents are very low, and matrix strengthening is on the weak side.
  4. P: 0.062%, acceptable, and will not cause phosphide eutectic embrittlement.

Composition summary: The carbon equivalent is slightly low, graphitization expansion is insufficient, and the casting itself has “insufficient self-feeding potential.” It can only rely more on riser feeding. Once the riser neck solidifies earlier than the hot spot, shrinkage porosity will appear below the riser, which corresponds exactly to the purple shrinkage porosity location in your ProCAST simulation.

II. Process level (resin sand + pressed-edge riser) — core causes

Although resin sand has higher rigidity than clay sand, the pressed-edge riser itself has inherent shortcomings:

First common cause: Premature solidification of the riser neck (most frequent)

A pressed-edge riser is a thin-gap feeding channel, and the gap is very thin. HT300 has a wide solidification interval, and resin sand dissipates heat quickly. The riser neck cools and solidifies first and seals off, so the riser molten iron cannot reach the casting hot spot. Even though the riser has not yet formed a shrinkage cavity, the feeding channel is already blocked, and the hot spot loses liquid supply, forming shrinkage porosity below the riser — exactly the defect in your simulation. In production, check whether the pressed-edge riser gap is thin. If not, rule out this first item.

Second common cause: Hot spot overlap

The transition between the flywheel hub and the rim is itself a hot spot. The pressed-edge gap happens to fall above this hot spot, so the hot spots superimpose, the solidification time is prolonged, and a longer feeding time window is required.

Third cause: Pouring temperature

Resin sand has low heat storage and cools quickly. If the pouring temperature is low (below 1320°C), the riser molten iron cools faster and the riser neck solidifies earlier; if the temperature is too high, overall liquid shrinkage increases.

4. Pressed-edge gap size design: A gap width that is too small and a gap length that is insufficient are the most common problems with pressed-edge risers. The pressed-edge gap is not better the narrower it is. For thick HT300 castings, the pressed-edge gap width must match the modulus. If the gap is too small, the feeding channel is very likely to be cut off.

5. Pouring sequence and mold filling: If top pouring or side pouring is used, the molten metal first fills the casting and the riser is filled last, so the riser temperature is low and it becomes a “cold riser,” and its feeding capacity is directly lost.

6. Resin sand gas generation and back pressure: If venting is poor, the mold cavity pressure rises, offsetting part of the graphitization self-feeding and amplifying the shrinkage porosity tendency.

III. Tiered corrective action plan

Plan 1: Composition fine-tuning (try first, smallest change)

Raise the carbon equivalent to 3.90–3.95: increase C to 3.25–3.32, control Si at 1.95–2.05. Purpose: increase graphitization expansion, use the self-feeding of gray iron, and reduce the feeding burden on the riser. Note: Si must not be too high, to prevent excessive ferrite and hardness/strength dropping below the lower limit of HT300. Supporting measure: strengthen inoculation, use stream inoculation, increase the amount of Type A graphite, make graphite fuller, and improve expansion. Keep S in the 0.045–0.055 range unchanged.

Plan 2: Pressed-edge riser/riser neck optimization (most targeted)

  1. Appropriately widen the pressed-edge gap and prolong the solidification time of the riser neck to ensure the channel does not seal before the hot spot solidifies. Do not widen blindly; if too wide, the riser and casting will fuse and cleaning will be difficult.
  2. Change the pressed-edge riser to a hot riser design: arrange the gating system so that molten iron enters the riser first and then flows into the casting through the pressed-edge gap, ensuring the riser has the highest temperature (sequential solidification: casting → riser neck → riser). This is the key to success or failure of the pressed-edge riser. Many flywheel pressed-edge riser failures occur because the molten iron first fills the flywheel and the riser is fed last, so the riser temperature is low and it becomes a cold riser.
  3. Check the pressed-edge riser volume: the riser modulus must be 1.1–1.2 times the modulus of the casting hot spot. HT300 has greater shrinkage than HT250, so the riser cannot be made according to HT250 experience.

Plan 3: Adjustment of pouring process parameters

  1. Pouring temperature: control at 1330–1350°C (resin sand HT300 flywheel large castings). Do not pour at low temperature and fast rate.
  2. Pouring speed: fill the mold smoothly, avoid air entrapment, and ensure the riser continuously receives hot molten iron for feeding.
  3. Resin sand: appropriately reduce the curing agent ratio to slow the cooling rate of the sand mold and ease the rapid cooling of the riser neck; at the same time ensure sand mold strength to prevent mold wall movement.

Plan 4: Alternative process

Keep the pressed-edge riser and add small chills at the hub hot spot to divide the hot spot, reduce the hot spot modulus, and lower the feeding requirement; or change the simple pressed-edge riser into a pressed-edge + blind riser composite riser for stronger feeding capacity.

IV. Pitfall reminders

For HT300 with Cr alloy, do not blindly rely on increasing the carbon equivalent to unlimitedly raise expansion. If carbon and silicon are too high, graphite becomes coarse, casting hardness becomes uneven, and machinability deteriorates. The core logic of the pressed-edge riser: the gap is a feeding channel, not simply a pool for holding iron. If the channel solidifies first, the riser becomes useless. This is the fundamental reason for “the riser looks full but the casting below has shrinkage porosity,” which matches your current phenomenon exactly.