I. Introduction
Ductile iron, with its excellent properties such as high strength, good toughness, wear resistance, and vibration damping, is widely used in industrial fields including automotive components, construction machinery, valve bodies and pipe fittings, and machine tool castings. The quality of graphite nodularization is the core key determining the mechanical properties of ductile iron, and the residual magnesium content is the core indicator for ensuring complete nodular graphite, eliminating flake graphite, and preventing nodularization decay.
Magnesium is the core active element in nodularization treatment. It is extremely chemically active with a very low boiling point, and in the high-temperature molten iron environment it is highly prone to vaporization, oxidation, and compound loss, collectively referred to in the industry as magnesium burn loss. Magnesium burn loss is unavoidable in production, but excessive fluctuation in burn loss will directly lead to batch quality defects such as poor nodularization, low nodularization grade, graphite distortion, and shrinkage porosity and inclusions in castings.
In actual production, magnesium burn loss is not caused by a single factor but is the result of the multi-dimensional combined effects of molten iron temperature, original composition, nodularizer quality, and process operation time. This article focuses on four core factors — nodularization temperature, base iron composition, magnesium oxide content in the nodularizer, and holding time after nodularization before pouring — and, combining casting process principles with workshop practical conditions, provides an in-depth analysis of their influence mechanisms on magnesium burn loss, providing a technical basis for stabilizing ductile iron production quality and reducing reject rates.
II. Effect of excessively high tapping/nodularization temperature on magnesium burn loss
The physical properties of magnesium determine its extreme sensitivity to temperature; the boiling point of pure magnesium is only 1107°C, far below the nodularization treatment temperature of molten iron. The conventional nodularization process temperature range for ductile iron is 1480°C–1520°C. Within this reasonable temperature range, magnesium can stably complete desulfurization, deoxidation, and graphite nodularization reactions, with controllable burn loss and stable residual magnesium content.
When the tapping and nodularization temperature exceeds 1530°C, magnesium burn loss increases exponentially. The high-temperature environment greatly increases the vapor pressure of magnesium. After the nodularizer is plunged into the molten iron, metallic magnesium vaporizes rapidly and escapes from the molten iron surface before it can fully diffuse and participate in the nodularization reaction, causing physical burn loss. At the same time, the oxidizing nature of high-temperature molten iron increases significantly, intensifying the oxidation reaction between magnesium and oxygen to form stable magnesium oxide waste slag, completely losing its nodularizing activity.
In addition, high temperature accelerates the oxidation consumption of rare earth elements in the nodularizer. The core role of rare earth elements is to encapsulate magnesium atoms, inhibit rapid magnesium burn loss, and delay nodularization decay. At high temperature, rare earths are consumed first, losing their protective effect on magnesium and further amplifying ineffective magnesium burn loss.
The chain quality problems caused by excessively high temperature are very prominent: with the same nodularizer addition amount, effective residual magnesium is insufficient, the casting develops vermicular graphite and flake graphite inclusions, and the nodularization grade drops from 2–3 to 4–5, directly causing the casting’s toughness and tensile strength to fail to meet standards and resulting in batch rejection. Therefore, production must strictly control nodularization temperature and prohibit over-temperature treatment.
III. Effect of base iron chemical composition on magnesium burn loss
The sulfur and oxygen contents of the base iron are the most core chemical factors affecting magnesium burn loss. Conventional elements such as carbon, silicon, and manganese have very little effect on magnesium burn loss and can almost be ignored.
Sulfur is the primary consuming element of magnesium and the biggest enemy of the nodularization process. Sulfur in the base iron is extremely active and will preferentially react chemically with metallic magnesium to form insoluble, stable magnesium sulfide inclusions. This reaction has priority over the graphite nodularization reaction and consumes a large amount of effective magnesium. The higher the sulfur content of the base iron, the more magnesium is lost to ineffective compound formation, and the magnesium burn loss rate rises linearly. If the base iron sulfur exceeds the standard, the conventional nodularizer addition amount cannot offset the sulfur consumption at all, ultimately leading directly to nodularization failure.
Next is the oxygen content of the molten iron. During melting, the molten iron dissolves a large amount of oxygen. Free oxygen reacts violently with active magnesium to form magnesium oxide slag, causing oxidative burn loss of magnesium. At the same time, excessive oxide slag and impurities in the molten iron continuously consume active magnesium, further aggravating the loss.
In actual production, inadequate melting process control, high impurity content in scrap steel, poor pig iron quality, and insufficient slag removal and deoxidation before tapping all lead to excessive sulfur and oxygen in the base iron. This is also the fundamental reason why, under the same formula, same nodularizer dosage, and same temperature conditions, the residual magnesium content fluctuates greatly between different heats and nodularization quality is unstable.
IV. Effect of nodularizer quality and magnesium oxide content on magnesium burn loss
The quality of the nodularizer directly determines the effective magnesium utilization rate, among which the magnesium oxide (MgO) content is the core indicator for judging nodularizer quality and is also the key factor causing false and hidden magnesium burn loss.
Metallic magnesium in the nodularizer is the only effective component with nodularizing activity, while magnesium oxide is an inert impurity formed by prior oxidation of magnesium. It has no nodularizing effect and cannot participate in the molten iron reaction, belonging to ineffective components. Inferior nodularizers have rough production processes and severe melting oxidation, with excessive magnesium oxide content. Under the same addition ratio, the effective metallic magnesium content is greatly reduced, equivalent to a disguised reduction in nodularizer dosage, indirectly creating the process illusion of “excessively high magnesium burn loss.”
At the same time, high-magnesium-oxide inferior nodularizers have a loose internal structure and a high powder proportion. Powdered nodularizer, upon contact with high-temperature molten iron, instantly floats, burns, and splashes, unable to sink into the deep molten iron for diffusion and reaction. Surface magnesium burns out rapidly, while deep molten iron is insufficiently nodularized, causing uneven nodularization quality between the upper and lower parts of the casting.
High-quality nodularizers strictly control magnesium oxide content, with stable proportions and uniform particles. They can both ensure the effective utilization rate of metallic magnesium and rely on rare earth components to inhibit magnesium burn loss. Conversely, low-priced inferior nodularizers appear to have lower cost, but magnesium loss is severe and quality fluctuates greatly, greatly increasing casting reject rates and resulting in higher overall production costs.
V. Effect of pouring time after nodularization on magnesium burn loss
Many production personnel only focus on magnesium burn loss at the moment of nodularization and ignore the continuous magnesium loss caused by the holding waiting time after nodularization, which is also the core cause of later nodularization decay.
After the nodularization treatment is completed, the residual active magnesium in the molten iron does not stop reacting. The trace residual oxygen and sulfur in the molten iron, as well as secondary oxidation from contact between the molten iron surface and air, continuously and slowly consume residual magnesium. The longer the holding time from the end of nodularization treatment to the completion of casting pouring, the more severe the continuous burn loss of magnesium, and the residual magnesium content continues to decline.
For short holding times (within 5 minutes), the magnesium decay amplitude is extremely small, with no obvious effect on nodularization quality; if the holding time exceeds 10 minutes, residual magnesium loss is obvious; if the holding time exceeds 15 minutes, nodularization decay is very likely to occur. This manifests as qualified nodularization in early metallographic testing, while castings poured later have coarse, distorted graphite nodules and flake graphite, with mechanical properties failing to meet standards.
In batch production and cross-operation of multiple molding lines, it is very easy for nodularized molten iron to accumulate and pouring to be delayed. Lax process control and poor coordination are the main human factors causing excessively long pouring times and excessive later-stage magnesium burn loss. Therefore, production must follow the principle of nodularize-and-pour, pour quickly and cool quickly, and strictly control the molten iron holding time.
In summary, magnesium burn loss in ductile iron production is the result of the combined action of four dimensions: physical temperature, chemical composition, raw material quality, and process operation. High temperature aggravates magnesium vaporization and oxidation; high-sulfur, high-oxygen molten iron consumes large amounts of magnesium through compound formation; high-magnesium-oxide nodularizers reduce effective magnesium utilization; and excessively long holding time after nodularization causes continuous decay and burn loss of magnesium.
To stabilize nodularization quality and reduce magnesium burn loss fluctuation, four major control points must be implemented: strictly control the optimal nodularization temperature of 1480–1520°C, perform desulfurization and deoxidation in advance to purify the molten iron, select low-magnesium-oxide high-quality nodularizers, and shorten the holding time after nodularization before pouring. Through full-process control, residual magnesium content can be effectively stabilized, nodularization defects can be eliminated, and the finished product rate and product stability of ductile iron castings can be greatly improved.