Hello everyone. Today we are going to talk about the issues that medium-frequency electric furnaces need to pay attention to in winter, to help our foundries take preventive measures.
Core contradiction in winter: Ambient temperature is low, and the furnace body, charge materials, tooling, and tapping ladles are all at low temperatures. Molten iron cools quickly and temperature drop fluctuates greatly, which easily induces nodularization decay, inoculation failure, porosity, cold shuts, and shrinkage porosity, while the risk of equipment freeze damage and electrical failures also rises. Let me explain this clearly in several parts:
I. Charge material management (most easily overlooked, a high-incidence source of rejects)
- Strictly prohibit charging materials with ice, snow, or frozen lumps
Snow, ice, and frozen moisture on the surface of shredded steel, returns, scrap steel, and pig iron rapidly vaporize after being charged, very easily causing explosive splashing. At the same time, the hydrogen content of the molten iron surges, and subcutaneous porosity and pinholes appear in batches in castings. The material yard should have a shed; snow-covered and frozen materials should be picked out first and preferentially dried and thawed; materials with thick ice should not be used at all.
- Do not directly add large amounts of cold charge at once
In winter, raw materials at room temperature may be 0°C or even below zero. Putting in a large amount of cold charge at one time causes the molten pool temperature to plummet, resulting in unstable melting and large composition fluctuations. Charging sequence: first add large pieces of easily melted material; after a molten pool forms, add cold charge in small batches.
- Keep alloys, inoculants, and nodularizers warm and stored properly
After ferrosilicon, ferromanganese, nodularizer, and inoculant absorb moisture, the moisture is carried into the molten iron. In winter, the warehouse should be moisture-proof and kept warm, and bags should be sealed; damp alloys must be dried at 200–300°C, cooled after drying, and then used. Once the nodularizer absorbs moisture, nodularization decay will be significantly aggravated.
II. Furnace lining and crucible maintenance (the risk of furnace lining cracking in winter is far higher than in summer)
- For newly rammed and rammed furnace linings, curing, drying, and baking at low temperature must be slowed down
At low temperatures, refractory materials cure slowly, and moisture does not easily escape. If a new furnace is baked according to the summer heating curve, the internal moisture expands rapidly and directly bursts the furnace lining and causes cracks. Reduce the heating rate during furnace baking, lengthen the holding time in the low-temperature section (100–300°C), and slowly remove free water.
- Keep the furnace warm during shutdown to prevent rapid cooling and cracking of the furnace lining
When melting ends at noon, do not directly cut off power and open the furnace to cool down. For long shutdowns, keep a small amount of molten iron in the furnace and hold at low power; for nighttime production stoppages, cover the furnace opening. Repeated alternation of hot and cold easily produces network cracks in the furnace lining, leading to iron leakage later.
- Cold furnace startup: do not go to full power and rapid heating right away; use stepped heating — first bake at low power for a period, then gradually increase power.
III. Control of molten iron temperature and pouring superheat (key point for ductile iron)
- Reserve sufficient temperature drop margin
At low ambient temperatures, the molten iron dissipates heat much faster than in summer throughout tapping, transfer, nodularization treatment, inoculation, and flow to the mold cavity. With the same tapping temperature, the temperature at the pouring position in winter will be 30–60°C lower. The longer the pouring time, the more obvious the pouring temperature drop.
Ductile iron: the tapping temperature should be appropriately raised, generally by 30–40°C; but it must not be overheated too much, as overheating will aggravate graphite flotation, oxidation, and burn loss.
- Strictly control the interval from tapping to pouring
In winter, molten iron cools quickly, and transfer ladles and pouring ladles dissipate heat quickly. Large ladles and small ladles must be preheated in advance. A cold ladle directly receiving molten iron causes a huge temperature drop and easily causes ladle lining peeling and gas entrainment. Pouring ladles, nodularization ladles, and slag-trapping ladles must be thoroughly baked before the shift, and the ladle wall must not feel icy cold to the touch.
- Increase temperature measurement frequency: measure temperature for every heat; do not judge by experience from the flame.
IV. Nodularization and inoculation process (a severe disaster area in winter for materials such as QT450-10)
- The nodularization reaction is greatly affected by temperature: if the temperature is on the low side, the nodularization reaction is insufficient and absorption rate is poor; if the temperature is too high, magnesium burn loss is too fast. Adjust the tapping temperature in winter to ensure a stable nodularization reaction window.
- Prefer stream inoculation and instantaneous inoculation: in winter, earlier-stage inoculation decay is faster, and large-ladle inoculation decays quickly. Try to rely on end-point stream inoculation to supplement inoculation and reduce chill and deterioration of graphite morphology.
- Do not put nodularizer and inoculant into a cold ladle bottom; preheat the ladle bottom in advance.
V. Cooling water and electrical systems (safety first)
- Freeze protection of cooling water is the top priority
For medium-frequency furnace water-cooled cables, inductors, capacitors, and water pipes, if water is stopped or remains during nighttime production shutdown, low temperatures will freeze it, causing pipes to burst and water-cooled cables to bulge and leak.
Nighttime shutdown: the circulating water pump must not be stopped casually; if the shutdown is long, all water in the pipes must be drained and purged.
Antifreeze: in severe cold workshops in the north, special antifreeze can be added to the circulating water pool in proportion, taking into account conductivity and corrosion resistance; ordinary automotive antifreeze must not be added casually.
- Check terminals and capacitors: at low temperatures, some insulating parts become more brittle, and large temperature differences easily cause condensation. Heavy fog and condensation in the workshop easily cause creepage, tripping, and arcing. Ensure good ventilation, moisture-proof the control cabinet, and do not let water vapor enter the distribution cabinet.
VI. Sand molds, tooling, and pouring support
- Clay sand, resin sand, and coated sand: in low-temperature environments, moisture in sand molds volatilizes more slowly; at the same moisture content, porosity is more likely in winter. The sand mold storage area should be freeze-proof, and sand molds should not be frozen hard.
- Cold molds and patterns: applying coating and filling with a low-temperature pattern easily causes chilling, and the risk of chill and cold shuts in thin-walled parts rises.
- Pouring rhythm: do not wait until the molten iron is cold before pouring; pour one mold as continuously as possible to reduce waiting.
VII. Special safety items
- Icy ground: remove ice and prevent slipping at the furnace front and pouring channels in a timely manner to prevent personnel falls and molten iron spill accidents.
- Strictly prohibit tools and sample ladles with water or ice from contacting molten iron; the explosion risk is extremely high.
- Before tapping molten iron and sampling, check the sample ladle and thermocouple protection tube; they must be dried and preheated.
Brief summary mnemonic
Three things for electric furnace melting in winter: no ice or snow in the charge, bake the furnace slowly, bake the ladle thoroughly and reserve temperature margin, and prevent condensation and freezing in the water cooling system.