Hello everyone, this is Lao Lu. These past two days, Lao Lu went to a company to troubleshoot high-carbon brake disc defects on site. I found some problems on site, and today I’ll put together a summary. I’d like to share these notes with everyone for discussion.
Nowadays, foundries producing automotive brake discs generally use static pressure molding lines and automatic pouring. It feels like the more automated equipment there is, the fewer casting efficiency problems and defects there should be. But if the people managing this advanced equipment are not professional, sometimes the more advanced the equipment, the more problems go undetected, and the more casting defects there are.
For example, today we are going to talk about porosity and slag hole problems in high-carbon brake discs.
Characteristics of static pressure molding lines: high sand mold compactness, relatively low sand mold permeability. High-carbon gray iron molten iron has good fluidity and its own characteristics of gas generation and oxidation. Brake discs have an annular structure with concentrated air duct cores, and subcutaneous porosity and slag holes are often concomitant.
To solve the problem, we must first distinguish the characteristic features of these two types of defects, and then troubleshoot item by item across melting, inoculation, sand cores, pouring, auxiliary materials, and equipment.
A quick distinction first: subcutaneous porosity is generally 1–4 mm below the surface, with round holes and smooth inner walls; slag holes are irregular in shape, containing slag, oxide scale, and silicate slag, mostly concentrated near the runners, above the air duct cores, at the disc surface R-angles, and on the upper surface of the casting.
I. Melting and molten iron
1. Raw material control
High-carbon brake disc batching mostly uses pig iron and carburizer. Impurities, rust, and oil contamination in carburizer, scrap steel, and returns are the source of oxidizing slag. Returns should be sorted separately and not mixed with coated sand or resin sand burned slag; select low-sulfur, low-ash, low-volatile graphite-based carburizer to avoid large amounts of gas generation and slag formation from inferior carburizer.
2. Tapping temperature and holding
Control the tapping temperature at 1490–1510°C. If the temperature is on the low side, deoxidation products and manganese sulfide slag do not easily float up; after tapping, hold the molten iron ladle for 60–90 s to give the slag time to float up. High-carbon molten iron must not be heated up and overheated violently; severe overheating causes the molten iron to absorb oxygen, and after pouring, CO subcutaneous porosity precipitates.
3. Deoxidation, degassing, and slag removal
During tapping, add silicon-manganese for preliminary deoxidation in the stream to reduce the oxygen content of the molten iron; put slag remover in the ladle, not just sprinkle it on the surface, stir to gather slag, and the slag must be skimmed clean. Many slag holes on static pressure lines occur because the floating slag in the ladle is not skimmed clean and is carried into the mold cavity in the stream.
4. Sulfur content control
For high-carbon brake discs, control S at 0.05–0.09%. If sulfur is too low, the inoculation reaction is poor and porosity is easily generated; if sulfur is too high, large amounts of manganese sulfide slag are generated and slag holes increase.
II. Inoculation system (very easily induces subcutaneous porosity)
Static pressure lines mostly use stream inoculation, which is also a high-frequency failure point:
- The inoculant addition amount must not be too large. Excessive addition precipitates large amounts of reaction gas, and the sand mold permeability is poor, so the gas cannot be discharged and forms subcutaneous porosity;
- Stream inoculation must be stable, avoiding interrupted flow and concentrated clustered feeding, which cause local excessive inoculation and concentrated gas;
- The inoculant must be dry. Damp inoculant directly introduces moisture, instantly generates gas, and causes batch subcutaneous porosity.
III. Sand mold and clay sand parameters (a shortcoming unique to static pressure lines: high compactness, limited permeability)
Static pressure lines compact at high pressure, and sand mold permeability is naturally lower than that of jolt molding. This is the core cause of porosity:
- Strict control of molding sand moisture: High moisture is the number one sand mold factor for subcutaneous porosity. High-carbon molten iron has a high temperature, and moisture vaporizes to produce large amounts of water vapor. Control moisture at 3.0–3.5%, with as little fluctuation as possible;
- Permeability: Regularly test molding sand permeability. Excessive dust and mud content in used sand directly blocks permeability; mud content should not be too high; used sand and hot sand should be cooled. Hot sand entering the molding machine causes the sand mold surface layer to dry and generate gas;
- Sand mold venting: For the annular structure of brake discs, specially add vent plugs at the upper mold, riser positions, and positions corresponding to the air duct cores. Static pressure line molds very easily neglect venting. If the sand mold is compacted too hard, gas can only be pressed into the subcutaneous layer of the casting; vent plugs must be cleaned regularly to prevent them from being blocked by sand and becoming ineffective;
- Sand mold surface stability: Reasonable coal powder addition. Too little coal powder makes it easy for molten iron to wet the sand mold, causing sand adhesion and slag entrainment; too much coal powder causes gas evolution to surge and porosity to break out. Select low-gas-evolution coal powder and control the total gas evolution.
IV. Resin sand air duct cores
The resin sand cores of ventilated discs are high-incidence defect locations:
- The sand core must be fully cured. If the core is “hard outside and soft inside,” the core interior continuously generates gas during pouring, and the gas rushes into the casting;
- Sand core coating: Select low-gas-evolution, high-temperature-resistant zircon powder coating. The coating should be uniform; do not apply thick accumulated coats. If the mold is closed before the coating is thoroughly dry, moisture + binder generate gas, and at the same time the coating peels off, forming coating slag holes;
- Sand core venting: Make vent channels at the core print, embed vent rope inside the core, and let the gas generated by the sand core be discharged from the core print; it must not run into the casting mold cavity;
- Mold closing purging: Before mold closing, use compressed air to blow clean floating sand and coating debris on the mold cavity and sand core surface. Many slag holes occur because loose sand and coating skins fall into the mold cavity. Close the mold as soon as possible after purging to prevent secondary dust fall.
V. Gating system and pouring process (key points for static pressure line automatic pouring)
- Runner design: For brake discs, prefer bottom pouring and step pouring for smooth mold filling, reducing molten iron turbulence, slag entrainment, and air entrainment. Lengthen the cross runner and add slag collection pockets to trap oxidizing slag in the slag collection pocket and prevent it from flowing into the casting; disperse the ingates to avoid single-point scouring of the sand core and sand mold;
- Pouring temperature: For high-carbon brake discs, pour at 1360–1400°C. If the temperature is on the high side, molten iron oxidation intensifies, oxidizing slag increases, and the reaction between molten iron and sand mold intensifies; if the temperature is on the low side, slag fluidity is poor, slag does not easily float up, and it gets stuck inside the casting;
- Pouring speed: The automatic pouring speed of the static pressure line must be matched. Do not fill the mold too fast, or the mold cavity gas cannot be discharged in time; nor too slow, or the molten iron surface oxidizes and forms slag;
- Pouring cup slag trapping: Add a slag trapping weir and filter screen to the pouring cup. The filter screen must be intact and undamaged. This is the last barrier to stop slag; if the filter screen is damaged, slag holes break out in batches.
VI. Equipment and on-site management
- Sand temperature: Ensure the used sand cooling system works, with sand temperature ≤45°C. Hot sand molding causes the sand mold surface layer to vaporize in advance, with large gas evolution;
- Mold closing sealing: After mold closing on the static pressure line, flashing and air leakage at the parting line also disrupt venting. The parting line sealing of the negative pressure/static pressure line must be in place;
- Timing: The interval between molding, mold closing, and pouring should not be too long, or the sand mold absorbs moisture and the sand core becomes damp again;
- Sampling distinction: First do comparative tests. With the same ladle of molten iron, switch to dry inoculant and strengthen slag skimming, and see whether slag holes decrease; separately add vent plugs and see whether subcutaneous porosity improves, to locate the root cause.
VII. Quick troubleshooting sequence
- Look at the defect location: concentrated near the sand core → prioritize checking sand core gas generation, coating, and core venting; concentrated on the upper surface and near the riser → insufficient mold cavity venting; distributed along the runner all the way → molten iron carrying slag, filter screen failure;
- First check the most problem-prone items: sand moisture, sand temperature, damp stream inoculant, whether the sand core is thoroughly dry, and the pouring cup filter screen;
- Then optimize: molten iron holding and slag removal, mold vent plug modification, runner slag collection structure;
- Finally fine-tune: pouring temperature, speed, and molding sand coal powder ratio.
VIII. Reminder
Do not blindly reduce sand mold compactness on static pressure lines to trade for permeability. A decrease in compactness will bring brake disc deformation and dimensional out-of-tolerance. The core approach is to control the total gas evolution + provide dedicated discharge channels for gas, rather than simply reducing compactness.